<kbd id="pqh4d5wu"></kbd><address id="pqh4d5wu"><style id="pqh4d5wu"></style></address><button id="pqh4d5wu"></button>

              <kbd id="ptod32sd"></kbd><address id="ptod32sd"><style id="ptod32sd"></style></address><button id="ptod32sd"></button>

                      <kbd id="labuvkrn"></kbd><address id="labuvkrn"><style id="labuvkrn"></style></address><button id="labuvkrn"></button>

                              <kbd id="84gs4az3"></kbd><address id="84gs4az3"><style id="84gs4az3"></style></address><button id="84gs4az3"></button>

                                      <kbd id="httk8zi1"></kbd><address id="httk8zi1"><style id="httk8zi1"></style></address><button id="httk8zi1"></button>

                                              <kbd id="sdafwg64"></kbd><address id="sdafwg64"><style id="sdafwg64"></style></address><button id="sdafwg64"></button>

                                                      <kbd id="35071sgy"></kbd><address id="35071sgy"><style id="35071sgy"></style></address><button id="35071sgy"></button>

                                                              <kbd id="7s06wx02"></kbd><address id="7s06wx02"><style id="7s06wx02"></style></address><button id="7s06wx02"></button>

                                                                      <kbd id="9bgozvhr"></kbd><address id="9bgozvhr"><style id="9bgozvhr"></style></address><button id="9bgozvhr"></button>

                                                                          威尼斯赌博网站

                                                                          消失模泡沫

                                                                          新聞分類

                                                                          產品分類

                                                                          聯繫我們

                                                                          威尼斯赌博网站

                                                                          聯繫人:隋經理

                                                                          手機: 13842554781
                                                                              18242478566

                                                                          電話: 0415-8190279

                                                                          郵箱: 768629865@qq.com

                                                                          網址:www.airjordanss.com

                                                                          地址:遼寧省鳳城市雞冠山鎮后街

                                                                          用於消失模泡沫鑄造專用泡沫珠粒的介紹(下)

                                                                          您的當前位置: 首 頁 >> 新聞資訊 >> 產品百科

                                                                          用於消失模泡沫鑄造專用泡沫珠粒的介紹(下)

                                                                          發佈日期:2016-08-09 00:00 來源:http://www.airjordanss.com 點擊:

                                                                          五、使用方法:


                                                                                消失模泡沫鑄造泡沫塑料模型生產過程中如下:


                                                                                原始珠粒 → 預發泡 → 乾燥、熟化 → 成型發泡 → 發泡塑料模


                                                                                1. 原始樹脂珠粒選用


                                                                                首先根據鑄件材質及對鑄件質量要求來選擇哪個品種 ,再根據


                                                                                鑄件的最小壁厚來選用珠粒規格 。一般選用的原始珠粒的粒徑小於或即是鑄件的最小壁厚的1/9 - 1/10。


                                                                                2.樹脂珠粒的預發泡


                                                                                消失模鑄造用珠粒的預發泡均採用間歇式預發泡機 。間歇式預發泡機有兩種即加壓式預發泡機和真空式預發泡機 。一般真空式預發泡機比加壓式預發泡機好 。兩種預發泡機的預發工藝參數可參考如下:


                                                                                a. 真空預發泡機操縱工藝參數:


                                                                                ①加樹脂 6秒


                                                                                ②預熱 見下表


                                                                                ③真空下注水 50-75ml/10秒


                                                                                ④大氣穩定 5秒


                                                                                ⑤真空穩定 20秒


                                                                                ⑥出料 45秒


                                                                                真空預發熱工藝參數

                                                                          加料量(克)夾套蒸汽壓力(Mpa)預發密度(克/升)
                                                                          共聚樹脂5003-50.15-0.18 18-20
                                                                          EPMMA5005-70.18-0.20 22-25
                                                                          EPS 5002-30.11-0.15 16-22


                                                                                b. 加壓式預發機


                                                                                EPS預發溫度爲100-105℃ ;


                                                                                共聚樹脂預發溫度爲105-115℃ ;


                                                                                EPMMA樹脂預發溫度115-120℃ ;


                                                                                珠粒的預發倍數一般由預發溫度和時間來控制。


                                                                                c. 預發珠粒的乾燥、熟化


                                                                                真空預發機不僅珠粒預發倍數高 ,珠粒粒徑均勻而且預發的珠粒是乾燥的 。若採用加壓式預發機預發 ,預發泡後的珠粒含水率高 ,需要用流化牀乾燥處理 ,乾燥風溫爲25-35℃  ,使珠粒含水率降至2%以下。


                                                                                經預發後的珠粒須存放一段時間後才能使用 ,這段時間稱爲熟化 。推薦的EPS熟化時間爲:

                                                                          堆積密度(克/升)15202530
                                                                          最佳熟化時間(小時)48-7224-4810-305-25
                                                                          最少熟化時間(小時)10520.5


                                                                                EPMMA及共聚樹脂預發珠粒熟化時間比上述EPS熟化時間推薦值要短。


                                                                                最佳熟化時間與環境溫度及空氣活動情況有關,熟化是否完成 ,可用珠粒的彈性好不好來判定。留意熟化溫度不宜太高 ,時間不宜太長 ,否則發泡劑損失過多影響成型發泡質量。熟化後珠粒要存放在密封的容器中 ,低溫貯存 。


                                                                                d. 成型發泡


                                                                                消失模泡沫塑料一般採用蒸缸成型和壓機成型兩種工藝:


                                                                                ① 採用蒸缸成型時,加熱蒸汽壓力(Mpa)

                                                                          EPS

                                                                          0.1

                                                                          共聚樹脂

                                                                          0.11-0.15

                                                                          EPMMA

                                                                          0.15-0.18


                                                                                保溫時間要根據模型大小、結構特點等通過試驗來確定 。


                                                                                ② 採用壓機成型典型的成型條件(模型尺寸爲50×200×200)爲


                                                                                模型材質密度(克/升) 通蒸汽時間(秒) 夾套蒸汽壓力(Mpa)冷卻時間


                                                                                (秒)


                                                                                最少 最大 正常


                                                                                共聚樹脂(20) 13 30 13 0.12-0.15 90


                                                                                EPMMA(26) 10 45 25 0.13-0.15 110


                                                                                EPS(24) 3 15 9 0.10 130


                                                                                成型發泡後模型要進行乾燥和存放(穩定化),模型在乾燥和存放過程中要收縮 。EPS模型收率爲0.4-0.8% ;EPMMA共聚樹脂模型收縮率爲0.2-0.4%;因此在成型模具設計時要考慮泡沫塑料模型的收縮率 。

                                                                          消失模泡沫

                                                                          相關標籤:消失模泡沫

                                                                          最近瀏覽:

                                                                          在線客服
                                                                          分享
                                                                          歡迎給我們留言
                                                                          請在此輸入留言內容,我們會盡快與您聯繫。
                                                                          姓名
                                                                          聯繫人
                                                                          電話
                                                                          座機/手機號碼